How Much LLDPE or mLLDPE to Blend Into LDPE Film

An LDPE blown film can take up to about 50% LLDPE before the bubble suffers; a shrink film keeps its shrink up to 30% with a Ziegler-Natta LLDPE and to about 50% with a metallocene partner. Up to that share, LLDPE adds puncture resistance and CD tear. Dart impact barely moves until LLDPE becomes the majority, and by then the film is LLDPE-based.

This answers the question for a film whose base is LDPE and where LLDPE goes in for toughness or clarity. Choosing the LLDPE grade itself by melt index, density and comonomer is covered in our LLDPE grade selection guide.

Typical LLDPE Share by Film Application

Shrink film carries 15–30% Ziegler-Natta LLDPE in the industrial and retail films that a shrink-film patent from ExxonMobil calls conventional, and 40–70% LLDPE in monolayer collation shrink film. Shrink film is the one LDPE-base film duty with published LLDPE shares.

Above 50% LLDPE, a collation film is no longer an LDPE-base film.

Collation and Shrink Film

An LDPE shrink film keeps its shrink with up to 30% Ziegler-Natta LLDPE, and with a metallocene partner up to about a 50/50 blend.

Above 30%, the ExxonMobil patent tested only its own metallocene resins. In the ExxonMobil patent’s 70 µm films blown at BUR 2.69, TD shrink held from 15% to 50% metallocene LLDPE and then roughly halved at 75%. If you plan more than 30% of a Ziegler-Natta LLDPE in a shrink film, test free shrink on trial film before committing to that share.

Free shrink at 150 °C of LDPE / metallocene LLDPE film, 70 µm, BUR 2.69 (%)
15% metallocene LLDPE
72 %
27 %
50% metallocene LLDPE
69 %
27 %
75% metallocene LLDPE
67 %
14 %
95% metallocene LLDPE
65 %
13 %
MD shrink
TD shrink

What Each Step of LLDPE Adds to the Film

Each step of LLDPE adds a different property at a different point: puncture and CD tear rise early, dart rises only past 50% LLDPE, and MD tear first falls. The clearest LDPE-base data are the worked examples in a Dow patent on LDPE blend compositions. The Dow patent’s monolayer films were 2 mil thick, blown at BUR 2.5 through a 70 mil (1.8 mm) die gap.

The Dow patent blended a 1.0 MI, 0.920 density octene Ziegler-Natta LLDPE (DOWLEX 2045G) into five LDPEs at 20%, 50%, 80%, 90% and 95% LLDPE.

Dart Impact and Puncture

Dart impact barely rises until LLDPE passes 50%; puncture starts rising sooner. Across all five LDPEs in the Dow patent’s 2 mil films, moving from 80/20 to 50/50 LDPE/LLDPE added only 6–27 g of dart. The table shows the full series for LDPE 132I.

LDPE / LLDPEDart drop impact (g)Puncture (ft-lbf/in³)
80 / 2017285
50 / 50190122
20 / 80241222
5 / 95302275
0 / 100388278

If dart is the property you are buying, a 20–50% LLDPE share adds little of it.

MD and CD Tear

The first LLDPE added to LDPE lowers MD tear, while CD tear climbs steeply. In the Dow patent, MD tear fell further from 80/20 to 50/50 with four of the five LDPEs. It recovered only once LLDPE was the majority.

Elmendorf tear, ASTM D1922, 2 mil film, BUR 2.5, LDPE 132I with DOWLEX 2045G LLDPE (g)
80/20 LDPE/LLDPE
224 g
377 g
50/50 LDPE/LLDPE
146 g
1022 g
20/80 LDPE/LLDPE
396 g
1186 g
5/95 LDPE/LLDPE
797 g
1023 g
Neat LLDPE
874 g
934 g
MD tear
CD tear

For a film that fails by tearing along the machine direction, a 20–50% LLDPE share makes MD tear worse. If CD tear is the weak side, the gain arrives early. CD tear in the Dow films peaked at 80–90% LLDPE and was still at or above neat LLDPE at 50/50.

Haze and Gloss

Adding LLDPE does not raise the haze of an LDPE film through most of the range, and past 50% LLDPE it often lowers it. On the LDPE-rich side, the LDPE grade has a far larger effect on haze than the share. Gloss behaves the same way in reverse.

Haze, ASTM D1003, 2 mil film, BUR 2.5, blends with DOWLEX 2045G LLDPE (%)
80/20 LDPE/LLDPE
13.5 %
38.8 %
9.8 %
50/50 LDPE/LLDPE
13 %
31.9 %
9.5 %
20/80 LDPE/LLDPE
8.2 %
15.3 %
7.2 %
LDPE 132I
LDPE 662I (autoclave)
AGILITY 1001

With an mLLDPE partner, blend films are smoother and less hazy than either pure resin.

What a Higher LLDPE Share Costs on the Line

On an LDPE line, die pressure and melt fracture limit the LLDPE share before bubble stability does, because the bubble stays stable up to about 50/50. How soon pressure becomes the limit depends on the die gap and on whether the resin carries a processing aid.

Melt Strength and Bubble Stability

The bubble does not lose LDPE’s stability until LLDPE passes about 50%. In the Dow patent’s blends with LDPE 132I, melt strength held flat from 20% to 50% LLDPE. It dropped by about 40% at 80% LLDPE.

Melt strength at 190 °C, LDPE 132I blended with DOWLEX 2045G LLDPE (cN)
80/20 LDPE/LLDPE
25 cN
50/50 LDPE/LLDPE
24.3 cN
20/80 LDPE/LLDPE
15 cN
10/90 LDPE/LLDPE
10.4 cN
5/95 LDPE/LLDPE
6.9 cN
Neat LLDPE
3 cN

Extruder Pressure, Motor Load and Die Gap

Extruder pressure rises mainly over the first half of the range, and on a narrow LDPE die it is the first limit you meet. The Dow patent ran its films at 250 lb/hr through a 70 mil die gap, with 800 ppm PPA in every blend. Screen pressure with LDPE 132I rose from 3,230 psi at 80/20 to 3,600 psi at 50/50 on that line. Screen pressure then stayed between 3,550 and 3,720 psi all the way to neat LLDPE.

A die built for LDPE has a much narrower gap, and the rise is larger there. On a die designed for LDPE, die pressure normally runs 3,000–4,000 psi. Neat 1 MI LLDPE raises it by at least 50%.

LLDPE also takes much more torque. Each step of LLDPE in the blend moves the motor load toward the extruder’s torque limit.

Melt fracture sets in sooner as the share rises, so sharkskin appears more readily as LLDPE goes up. A typical LDPE die gap is about 1 mm (0.040 in), while neat LLDPE runs at 2–2.5 mm (0.080–0.100 in), depending on output.

Raise the LLDPE share in steps on trial runs and log die pressure, motor load and the film surface at each step. Sharkskin on a 1 mm gap, or pressure at your extruder’s limit, marks the share at which the die gap needs to open toward the LLDPE range.

Does mLLDPE Change the Ratio?

At 15–20% in LDPE, an mLLDPE partner gives about the same toughness as a Ziegler-Natta LLDPE, and its gain at that share is clarity. The puncture advantage opens from 30% upward. In the ExxonMobil patent’s 50 µm films at 70/30 LDPE/partner, puncture energy was about 2.5 times higher with the metallocene resin. Clarity improved at every share.

Puncture resistance damaging energy of LDPE-base shrink film by partner type (mJ/µm)
85/15 LDPE/partner, 70 µm, BUR 2.69
38.3 mJ/µm
39.3 mJ/µm
70/30 LDPE/partner, 170 µm, BUR 4.5
104 mJ/µm
87.4 mJ/µm
70/30 LDPE/partner, 50 µm, BUR 2.2
96 mJ/µm
37.4–38.4 mJ/µm
Metallocene LLDPE partner
Ziegler-Natta LLDPE partner

These are the patent applicant’s own metallocene resins, not a generic mLLDPE. The patent claims them with a melt index ratio (I21.6/I2.16) of 30 to 80, which processes more easily than a typical narrow-distribution mLLDPE. Some metallocene grades run high extruder pressure, use more energy and give poorer bubble stability, so with those grades the line limits above arrive at a lower share.

Choose an mLLDPE partner when the blend will carry 30% or more and puncture is the goal, or when clarity is worth its price at any share. At 15–20% for toughness alone, a Ziegler-Natta LLDPE does the same job.

Newsletter Updates