What Counts as an HDPE 6095 Equivalent for Film

A 6095 equivalent for film is a high molecular weight HDPE film grade whose high-load melt index (190 °C/21.6 kg) and density match the 6095 your spec was written from. OQ’s Luban 6095 sheets print a high-load melt index of 10.5 g/10 min at 190 °C/21.6 kg and a density of 0.952 g/cm³. The comonomer does not have to match. Film properties such as dart and tear count only when both sheets blew and tested their film the same way.

This applies to replacing a 6095 on a blown-film line already running sacks and bags. Before any comparison, find out which 6095 the spec describes, because more than one grade carries the number.

Which 6095 Does Your Spec Describe?

Your spec describes one of at least three grades sold as 6095, and the data sheet it was copied from shows which one. Two of them share the name DGDX-6095:

  • OQ Luban DGDZ-6095: a hexene copolymer. OQ now sells it as Luban HD-F5211, with “Legacy name: Luban DGDZ-6095” on the August 2025 sheet and the same property rows as the 2021 DGDZ-6095 sheet.
  • OQ Luban DGDX-6095: a butene copolymer. Its data sheet prints the same melt index, high-load melt index and density as DGDZ-6095.
  • PetroChina Dushanzi DGDX-6095: a butene-1 copolymer. The Dushanzi DGDX-6095 specification tests to PetroChina’s Q/SY enterprise methods.

A spec that reads only “DGDX-6095” therefore does not identify the producer. Look at the sheet the spec was copied from. An OQ sheet carries the Luban name, ASTM methods and a melt index at both 2.16 kg and 21.6 kg. A PetroChina Dushanzi sheet carries Q/SY methods and a 21.6 kg figure alone.

The resin rows cannot tell OQ’s two 6095s apart, because OQ prints identical values for both. Only the comonomer line on the sheet (“Hexene High Density Resin” or “Butene High Density Resin”) does.

The Melt Index and Density a 6095 Equivalent Has to Match

Match the high-load melt index at 190 °C/21.6 kg and the density. OQ’s 6095 sheets print a high-load melt index of 10.5 g/10 min at 190 °C/21.6 kg and a density of 0.952 g/cm³ (ASTM D792).

Check the load printed beside every flow figure before you compare it:

  • ExxonMobil: prints a melt flow rate at 190 °C/5.0 kg and a high-load melt index at 21.6 kg, with no 2.16 kg value.
  • Formosa: prints rows labelled “Melt Index” and “HLMI” with no load or temperature beside either.
  • LyondellBasell and SCGC: print a 2.16 kg melt flow rate and no high-load figure, so their sheets cannot settle the 21.6 kg match. Ask the producer for the high-load value.

Neither number identifies the grade on its own. OQ’s Luban DGDX-6097 prints the same melt indices as the 6095 and differs only in density: 0.948 g/cm³ against 0.952. A spec that quotes the melt indices without the density could describe either OQ grade.

None of these sheets prints a tolerance. OQ, ExxonMobil and Formosa all label their values typical properties. Judge a substitute against where comparable grades sit: the producer sheets in the table below span a high-load melt index of 8.5 to 10.5 g/10 min and a density of 0.949 to 0.954 g/cm³. A candidate outside that spread has no published peer among these grades, so qualify it on a line trial at your own gauge before treating it as a 6095.

Which Grades Sit in 6095’s Melt Index and Density Band

SABIC F00952 and ExxonMobil HD 5295HL and HD 5290HLFL sit closest to the 6095: each prints a density of 0.952 g/cm³ and a high-load melt index of 9 to 9.5 g/10 min at 21.6 kg. Formosa E924 sits at the low edge of density. LyondellBasell L5005 and SCGC H5604F print no high-load figure, so their sheets alone cannot place them.

Grade (producer)Melt index, 190 °C/2.16 kg (g/10 min)High-load melt index, 190 °C/21.6 kg (g/10 min)Density, g/cm³ (method)
Luban DGDZ-6095 / DGDX-6095 (OQ), reference0.0510.50.952 (ASTM D792)
F00952 (SABIC)0.0590.952 (ASTM D1505)
HD 5295HL (ExxonMobil)not printed9.50.952 (ASTM D1505)
HD 5290HLFL (ExxonMobil)not printed9.00.952 (ASTM D1505)
Formolene E924 (Formosa)0.04 (load not printed)8.50 (“HLMI”, load not printed)0.949 (ASTM D1505)
Alathon L5005 (LyondellBasell)0.06not printed0.949 (method not shown)
H5604F (SCGC)0.04not printed0.954 (ASTM D1505)

A grade in this table qualifies for a trial on your line as a 6095 substitute; the numbers do not show it will run the same.

Does the Comonomer Have to Match?

No. At the 6095’s density the published data show only small differences between a butene and a hexene grade. OQ’s DGDZ-6095 (hexene) and DGDX-6095 (butene) share melt index, high-load melt index and density:

Property (OQ typical value)DGDZ-6095, hexeneDGDX-6095, butene
Flexural modulus, 1% secant, molded bar (MPa)11801160
Film tensile stress at yield, MD/TD (MPa)35/2933/27
Film tensile stress at break, MD/TD (MPa)53/6447/63
Film tensile strain at break, MD/TD (%)230/380180/390

If a substitution shows any difference, expect it when butene replaces hexene, in MD tensile and tear. A published comparison of hexene and butene LLDPE at similar density and melt flow found the hexene cast film higher in tensile strength, tear and impact.

Reading 6095 Film Properties Side by Side

Compare two sheets’ film properties only when gauge, blow-up ratio and frost line height match, and only when the row is measured on film. OQ blows its 6095 test film at a frost line height of 1080 mm and a blow-up ratio of 4:1, and states the gauge only on the dart row: 12.7 µm. Other producers test differently:

  • ExxonMobil: film properties on 15 µm film at a blow-up ratio of 4:1 and a frost line height of 9 times the die diameter.
  • Formosa: 0.50 mil film at a blow-up ratio of 4.0:1 and a stalk height of 8 times the die diameter, with dart reported in g/mil.

Do not convert between these. In a published study of HMW-HDPE blown film, dart, MD tear and TD tear each shifted with frost line height at a fixed resin and a fixed 4:1 blow-up ratio. One resin gave higher dart in its thinner films, so dividing dart by thickness does not put two gauges on the same footing.

The flexural modulus on OQ’s 6095 sheets is not a film property. OQ measures its 1% secant figure on molded bars. Do not set it beside a 2% secant figure on another sheet.

Treat the dart on OQ’s DGDX-6095 sheet as unconfirmed. OQ’s DGDX-6095 sheet prints 1117 g at 12.7 µm, while OQ’s DGDZ-6095 prints 128 g and OQ’s lower-density butene DGDX-6097 prints 127 g under the same test footnote. Confirm the DGDX-6095 dart with OQ before you use it, and do not read it as a butene advantage.