The ABS grade that holds impact strength at low temperature is the producer’s high-impact grade. Confirm it on the data sheet’s notched-impact line at −30 °C. Compare candidate grades on that line in one test standard.
The answer depends on how cold the part is when it takes a knock. Down to about −30 °C, buy a high-impact ABS and choose between grades on their printed −30 °C figures. Colder than that, start from the same high-impact grade and get a figure at your own temperature: a value from the producer, or an impact test on moulded parts at that temperature.
Which ABS Grade Family Keeps Impact in the Cold
High-impact ABS is the grade family that keeps the most notched impact in the cold. ABS is sold as general-purpose, high-impact, heat-resistant, flame-retardant and plating grades (the families are compared in types of ABS plastic).
In the INEOS Terluran grade flyer, Charpy notched impact (ISO 179/1eA) at −30 °C is 13 kJ/m² for the high-impact Terluran HI-10 and 8 kJ/m² for the general-purpose Terluran GP-22.
Each Terluran grade keeps about 37 % of its 23 °C Charpy value at −30 °C, so compare grades on the cold figure itself rather than on the percentage they lose.
Read the Low-Temperature Izod on the Data Sheet
The figure that shows cold impact is the notched-impact row with a low test temperature in its name, such as “Izod Notched Impact Strength, −30 °C”. The 23 °C row is a different figure. Producers print one row per test temperature: the Terluran HI-10 ASTM data sheet lists notched Izod at 23 °C, −18 °C and −30 °C as three separate rows.
Some sheets give the cold value as Charpy notched impact (ISO 179/1eA) instead of Izod, as the Terluran flyer does. An impact line with no test temperature printed is not a cold figure. Ask the producer for the cold line before comparing that grade.
On sheets that use ISO methods, the cold line is usually at −30 °C. On ASTM sheets, read the temperature in each cold row’s name, because it varies from sheet to sheet: the HI-10 ASTM sheet prints −18 °C and −30 °C. If your part takes impact colder than the coldest row on the sheet, ask for a value at your temperature instead of reading one off the trend.
Compare two grades only within one standard. ASTM D256 reports notched Izod in J/m (or ft·lb/in). ISO 180 reports it in kJ/m². No fixed factor converts one into the other. For Terluran HI-10, the ASTM D256 figure divided by the ISO 180/A figure is 12.5 at 23 °C (448 J/m against 36 kJ/m²) but 8.4 at −30 °C (117 J/m against 14 kJ/m²).
Charpy and Izod count as two standards even when both print kJ/m²: the HI-10 ISO sheet gives 13 kJ/m² Charpy and 14 kJ/m² Izod at −30 °C. When two sheets use different standards, ask one producer for its figure in the other’s standard at the same temperature.
Check the standard on each row, not on the block heading. The SABIC CYCOLAC MG47 data sheet gives notched Izod at 23 °C as 320 J/m by ASTM D256, and directly below it gives the −30 °C value as 8.0 kJ/m² by ISO 180/1A. That −30 °C row pairs with the sheet’s ISO 180/1A row at 23 °C, 22 kJ/m², not with the 320 J/m above it.
On ASTM sheets, check the specimen thickness as well. The Elix ABS E401 data sheet gives notched Izod at 23 °C as 390 J/m on a 3.2 mm bar and 290 J/m on a 6.4 mm bar. Compare cold rows from two sheets only at the same thickness.