How to Compare Dart Drop Figures Across PE Film Datasheets

Two dart drop figures can share a column only when both sheets used the same dart method (A or B), tested film of nearly the same gauge blown under similar conditions, and measured the resin on its own. Even then, both are typical values, not guaranteed ones.

These checks tell you whether two PE film grades can be ranked on their sheets. They do not predict the dart your own film will reach on your line, because each producer tests on its own reference film.

Check Whether Each Sheet Used Method A or Method B

Read the letter after the standard number: “ASTM D1709A” or “D 1709/A” means Method A. A Method A figure cannot be compared directly with a Method B figure.

The two methods drop different darts from different heights, and each covers its own range of failure mass:

Standard and methodDart head diameterDrop heightFailure mass range
ASTM D1709, Method A38.10 ± 0.13 mm0.66 ± 0.01 mabout 0.05 to 6 kg
ASTM D1709, Method B50.80 ± 0.13 mm1.52 ± 0.03 mabout 0.3 to 6 kg
ISO 7765-1, Method A38 ± 1 mm0.66 ± 0.01 mabout 0.05 to 2 kg
ISO 7765-1, Method B50 ± 1 mm1.50 ± 0.01 mabout 0.3 to 2 kg

Several sheets print only the standard number, with no letter. When the letter is missing, the failure mass range gives a rough guide. Method B starts at about 0.3 kg under both standards, so a gram figure below about 300 g sits under Method B’s range and most likely came from Method A. Above 300 g the two ranges overlap and the figure alone does not tell you, so ask the producer which method its lab ran.

Compare Only at the Same Film Thickness

Dart figures can be compared only when the test films are close in gauge, and dividing each figure by its thickness does not fix a gauge mismatch. ISO 7765-1 treats data as comparable only within ±10 % of the nominal thickness. For ASTM D1709 figures, the usual limit is a thickness difference of no more than 25 %.

Read the gauge before the figure. OQ’s DGDZ-6095 sheet tests at 12.7 µm and ExxonMobil’s HD 5295HL sheet at 15 µm. ExxonMobil’s HD 5295HL test film is about 18 % thicker than OQ’s DGDZ-6095 test film, which is inside the 25 % limit for D1709 figures.

Per-thickness figures stay tied to one gauge as well. Formosa’s E924 sheet prints g/mil measured on 0.50 mil film, and GAIL’s LLDPE table prints g/µm measured on 25 µm film. To set a g/mil figure beside a g/µm figure at the same test gauge, divide the g/mil figure by 25.4, since 1 mil is 25.4 µm. Do not use either figure to estimate grams at another gauge.

Match the Film-Making Conditions Behind the Figure

Blow-up ratio, frost line height, die gap and the type of line all have to be close, because each one changes the dart of the same resin at the same gauge. Treat a different blow-up ratio or frost line height as a different test film, even when the gauge matches.

Dart drop impact, ASTM D1709 (g): one HDPE/LLDPE blend, about 10 µm blown film, one industrial line, by neck height
Neck height 11.2 × die diameter (9.5 µm)
297.5 g
Neck height 8.8 × die diameter (9.7 µm)
300.5 g
Neck height 5.8 × die diameter (9.9 µm)
106.4 g

Check these items in each sheet’s test-film footnote:

  • Blow-up ratio: the blown-film LLDPE sheets cited in this article test at 2.5:1 and the HMW-HDPE sheets at 4:1. A figure at another ratio describes a different film.
  • Frost line or stalk height: OQ’s DGDZ-6095 sheet gives 1,080 mm, and ExxonMobil’s HD 5295HL sheet gives 9 times a 120 mm die, the same height. OQ’s LL-F1802 sheet states only gauge and blow-up ratio, which leaves a large variable open.
  • Die gap and output: ExxonMobil’s C6LL 2042.48 sheet states line size, die gap, melt temperature and rate. When a sheet omits a condition the other sheet states, do not rank the two figures; ask the producer for its test-film conditions first.
  • Blown or cast line: ExxonMobil’s C4LL 1018.32 figure comes from a cast-film line, so it does not belong in a column of blown-film figures.

Pure Resin or Blend

Most sheets measure dart on film of the resin alone, and a sheet that used a blend marks it next to the value. Borealis’s blown-film summary sheet, for example, flags some values “in blend with LD”. A neat-resin figure ranks resins for 100 % film only. The ranking can change once you add LDPE.

Dart drop impact, ASTM D1709 (g): 2 mil blown film, one LLDPE alone and with each of five LDPEs (examples in Dow patent US 10,287,423)
LLDPE alone
388 g
5 % LDPE (five LDPEs)
283–343 g
10 % LDPE (five LDPEs)
250–337 g
20 % LDPE (five LDPEs)
214–244 g

Read the footnote row by row. OQ’s LL-F1802SA sheet mentions a 10 % LDPE addition, but only for its optical rows. Its dart row was measured on film of the grade alone.

Typical Value or Guaranteed Minimum

The dart figure on a PE film datasheet is a typical value. A gap between two sheets therefore compares two producers’ reference films and is no guarantee for the lot you receive.

A page headed “specification” does not change this. GAIL’s LLDPE specification table prints one dart value per grade with no limit. A guaranteed property carries a limit sign, such as ± or ≥.

Some sheets print a bound in place of a value. ExxonMobil gives “< 60 g” for C6LL 2042.48 and for C4LL 1018.32. Two “< 60 g” figures cannot be ranked against each other.

ASTM D1709 or ISO 7765-1

An ASTM D1709 figure can be compared with an ISO 7765-1 figure when the method letter and the gauge match. When an ASTM sheet sits beside an ISO sheet, use ISO’s tighter ±10 % thickness window as a rough guide. ASTM describes D1709 as technically equivalent to ISO 7765-1:1988.

A Chinese sheet that cites GB/T 9639.1-2008, China’s dart standard, can be read as an ISO 7765-1 figure.

Read the standard on every row, even within one producer’s literature. Borealis’s blown-film summary sheet lists ASTM D1709/A for its Anteo family and ISO 7765-1 for its other families.

Grams or Joules

A dart figure in grams cannot be compared with an impact figure in joules. A gram figure is the dart mass at 50 % failure from ASTM D1709 or ISO 7765-1. A joule figure on a PE film sheet comes from a different test: a puncture test such as ISO 7765-2, which records force and deflection, ASTM D5748, or a producer’s own method.

Compare joule figures only with joule figures from the same test and on the same basis. Borealis prints J on FB2230 and J/mm on FB1490.

Do not convert a gram figure to joules either, not even by multiplying the dart mass by its drop height: the result is a different measurement from another sheet’s puncture energy.

Newsletter Updates

Enter your email address below and subscribe to our newsletter